1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B
Production specification
Square-shape steel standard Download
Plate steel standard Download
Billet standard Download
Flat bar standard Download
wire standard Download
tube standard Download
pipe standard Download
Forging standard Download
casting standard Download
sheet standard Download
round bar standard Download
coil standard Download
Bar stock standard Download
profiled bar standard Download
1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B
Designation by Standards
Brand Name | LH No. | Mat. No. | DIN | EN | AISI |
PK12NB | 936 | 1.4580 | X6CrNiMoNb17-12-2 | - | 316 Condition B |
Chemical Composition (in weight %)
C | Si | Mn | Cr | Mo | Ni | V | W | Others |
max. 0.08 | max. 1.00 | max. 2.00 | 17.50 | 2.25 | 12.00 | - | - | Nb=10 x C - 1 |
Description
This austenitic stainless steel has an increased molybdenum content to increase its resistance to corrosion when compared to other 300 series alloys. It will resist scaling at temperatures up to 871oC and maintains good mechanical properties and ductility.
Applications
Widely used in industry, it was initially designed for paper mill machinery. It has been used in marine environments and a wide variety of general industrial components. Component parts for the cellulose, paper, oil, soap and textile industry, production of paints, meat processing industry, breweries, dairies and for surgical instruments.
Physical properties (avarage values) at ambient temperature
Modulus of elasticity [103 x N/mm2]: 200, 186 (200oC), 172(400oC)
Density [g/cm3]: 7.98
Thermal conductivity [W/m.K]: 15.0
Electric resistivity [Ohm mm2/m]: 0.75
Specific heat capacity[J/g.K]: 0.50
Coefficient of Linear Thermal Expansion 10-6 oC-1
20-100oC | 20-200oC | 20-300oC | 20-400oC | 20-500oC |
16.5 | 17.5 | 18.0 | 18.5 | 19.0 |
Hardening
Harden from a temperature of 1020-1100oC followed by water or oil quenching. Structure is austenite with small ferrite component.
Mechanical properties in solution-annealed condition
Hardness: 130-190 HB
0.2 % proof stress: 215 N/mm2
Tensile strength: 510-740 N/mm2
Elongation: min. 35% (for d<=160, longit.)
Notch impact energy (ISO-V): min. 85 J
Mechanical Properties At Elevated Temperatures
Temperature | 50oC | 100oC | 150oC | 200oC | 250oC | 300oC | 350oC | 400oC |
0.2 % proof stress in N/mm2 | 206 | 186 | 177 | 167 | 157 | 145 | 140 | 135 |
Forging
Hot forming temperature: 1200-900oC.
Machinability
Low speeds and constant feeds will minimize this alloy's tendency to work harden. Tougher than 304 stainless with a long stringy chip, the use of chip breakers is recommended.
Corrosion Resistance
Resistant to a wide variety of marine environments, salts, dilute nitric, acetic and sulfuric acids.
Welding
All common fusion and resistance methods except oxyacetylene welding have proven successful. Use AWS E/ER316 or 316L filler metal for best results.
Cold working
Shearing, stamping, heading and drawing can be successfully performed . To remove internal stresses, a post-work annealing is recommended.
Related hot word search:1.4580 DIN X6CrNiMoNb17-12-2 1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B round bar,1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B forging,1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B sheet,1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B coil,1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B flat bar,1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B pipe,1.4580, DIN X6CrNiMoNb17-12-2, AISI 316 Condition B Lrregular